Alumina and Zirconia Properties
Note : Ceramic properties can vary with the manufacturing method
|
|
Al2O3 |
ZrO2 |
Physical Properties |
|
|
|
Chemical composition |
99.8% Al203 |
+3% Y203 |
|
Crystalline structure |
Corundum |
Tetragonal |
|
Sintered grain size (microns) |
1- 3 microns |
< 0.5 micron |
|
Sintered density |
3.92 g/cm3 |
6.03 g/cm3 |
|
water absorption |
0 |
0 |
Mechanical properties at 20 °C |
|
|
|
Vickers hardness (Hv 0.1) |
1800-2000 |
1300-1500 |
|
Bending strength (N/mm2) |
200-600 |
1000-1500 |
|
Young's modulus (N/mm2) |
3.8X105 |
2.0x105 |
|
Fracture toughness: K1c 1/2 (Mpa.m) |
4-5 |
8-15 |
Thermal Properties |
|
|
|
Dilatation coef. From 20 °C to 2000 °C |
8.4x10 -6 |
8.0x10-6 |
|
Thermal conductivity at 20 °C (W/m.K) |
40 |
2.5-2.8 |
|
Thermal Shock resistance (°C) |
200 |
400 |
|
Electrical Properties |
|
|
|
Resistivity at 20°C (ohm .cm) |
>1014 |
>1014 |